Zirconium is a reactive metal; it has a high affinity for oxygen and as such forms a protective oxide film that enables it
to perform well in a wide variety of conditions.
Atomic No. 40
Atomic Wt. 91.22
Specific Gravity 6.51
Melting Point 1852 degree
Atomic No. 40
Atomic Wt. 91.22
Specific Gravity 6.51
Melting Point 1852 degree
Coefficient of Thermal Expansion 5.8 X 10-6/K
Specific Heat 0.066 cal/g/K
Ultimate Tensile Strength (Room Temperature, Annealed) 55 ksi
Yield Tensile Strength (Room Temperature, Annealed) 30 ksi
Poisons Ratio 0.35
Modulus of Elasticity 14.4 X 106 psi
Stress Relief Temperature 565 degree
Specific Heat 0.066 cal/g/K
Ultimate Tensile Strength (Room Temperature, Annealed) 55 ksi
Yield Tensile Strength (Room Temperature, Annealed) 30 ksi
Poisons Ratio 0.35
Modulus of Elasticity 14.4 X 106 psi
Stress Relief Temperature 565 degree
tem Name
|
Zirconium pipe tube
|
Material
|
Pure Zirconium and Alloy Zirconium
|
Grade
|
R60702,R60704,R60705
|
Specification
|
According to your request or draiwng or sample
ASTM B523/ASME SB-523, ASTM B658/ ASME SB-658, DIN 2462 D3/T3 or closer
|
Applications
|
industry, metal smelting etc.
|
Chemical composition
Grade
|
Element composition(%)<
| ||||||||
Zr+Hf
|
Hf
|
Fe+Cr
|
Sn
|
H
|
N
|
C
|
Nb
|
O
| |
R60702
|
99.2
|
4.5
|
0.20
|
--
|
0.005
|
0.025
|
0.05
|
--
|
0.16
|
R60703
|
98
|
4.5
|
--
|
--
|
--0.005
|
0.025
|
--
|
--
|
--
|
R60704
|
97.5
|
4.5
|
0.20~0.40
|
1.0~2.0
|
0.005
|
0.025
|
0.05
|
--
|
0.18
|
R60705
|
95.5
|
4.5
|
0.2
|
--
|
0.005
|
0.025
|
0.05
|
2.0~3.0
|
0.18
|
R60706
|
95.5
|
4.5
|
0.2
|
--
|
0.005
|
0.025
|
0.05
|
2.0~3.0
|
0.18
|
Mechnical Properties:
Material
|
State
|
Rm(≥)/MPa
|
Rp0.2(Pa
|
A50mm(≥)/%
|
Zirconium 702
(UNS R60702)
|
annealed
|
379
|